Hardness(shore A) | 67 | 65 | 65 | 64 | 63 | 62 |
Tensile strength(Mpa) | 12.8 | 13.4 | 13.2 | 12.6 | 12.8 | 12.6 |
Elongation(%) | 275 | 360 | 335 | 335 | 335 | 335 |
Compression set(%) | +27 | +27 | +28 | +29 | +28 | +29 |
Ozone-resistance(50pphm, 40°C, 3day) | No Crack | No Crack | No Crack | No Crack | No Crack | No Crack |
Low temperature resistance(TR-10) | −47.7 | −48.3 | −49.6 | −50.9 | −52.7 | −53.0 |
Heat resistance (120°C, 70hr) | Hardness change(%) | +10 | +12 | +10 | +11 | +10 | +10 |
Tensile strength change(%) | −6.3 | −7.5 | +13.9 | +17.5 | +3.9 | +2.4 |
Elongation change(%) | −40 | −50 | −38.8 | −38.8 | −45.1 | −44.8 |
Oil resistance (ASTM IRM 901, 120°C, 70hr) | Hardness change(%) | +4.0 | +4.0 | +4.0 | +5.0 | +5.0 | +5.0 |
Tensile strength change(%) | +3.9 | +3.7 | +12.1 | +14.3 | −2.3 | +22.2 |
Volume change(%) | −3.4 | −4.3 | −5.2 | −5.2 | −7.0 | −8.5 |
Oil resistance (ASTM IRM 903, 120°C, 70hr) | Hardness change(%) | −6.0 | −5.0 | −6.0 | −6.0 | −5.0 | −5.0 |
Tensile strength change(%) | −12.5 | −9.0 | −6.8 | −10.3 | +1.6 | +6.3 |
Volume change(%) | +20 | +18.3 | +19.0 | +16.7 | +15.4 | +13.8 |