Table 11. Mechanical Properties of the Compounds by Changing Sulfur/CBS Content

T-3 T-4 T-5 T-6 T-7
Hardness (Shore A) 69 70 71 72 73
M300% (kgf/cm2) 90.8 115.3 134.3 154.9 170.7
Elongation at break (%) 560 500 440 410 370
Tensile strength (kgf/cm2) 240 240 230 240 230
Toughness (kgf*%/cm2) 55,300 51,100 43,200 41,400 35,900