Table 2. Tensile and Tear Strength Properties of SBR Rubber Composites
Compounds | Tensile strength (MPa) | Modulus at 150% elongation (MPa) | Elongation at break (%) | Tear Strength (MPa) |
Control | 2.75 ± 0.20 | 0.65 ± 0.08 | 275 ± 5 | 1.97 ± 1.13 |
C30 | 17.21 ± 1.08 | 1.59 ± 0.19 | 532 ± 11 | 10.50 ± 0.74 |
S30 | 11.64 ± 0.88 | 2.15 ± 0.20 | 331 ± 11 | 5.83 ± 0.67 |
C50 | 20.60 ± 1.49 | 3.09 ± 0.09 | 492 ± 25 | 23.66 ± 2.96 |
S50NT | 20.70 ± 4.42 | 1.40 ± 0.04 | 675 ± 67 | 8.12 ± 1.52 |
S50 | 17.50 ± 3.42 | 2.67 ± 0.31 | 369 ± 48 | 21.63 ± 1.94 |
S60 | 13.59 ± 2.15 | 3.64 ± 0.11 | 261 ± 8 | 34.53 ± 4.95 |