Types | CB-filled NR/BR blend compounds (Dump temp.: 140°C 145°C) | ||||
---|---|---|---|---|---|
NR/BR/CB-C (5:30) | NR/BR/CB-C (11:00) | NR/BR/CB-Y | |||
step | Time (min:s) | Action | |||
first stage | 0:00 | Add Rubber (NR/BR) | Add NR/CB MB and BR/CB MB | ||
1:30 | Add ½ (CB + oil) | - | |||
2:30 | Add ½ (CB + oil) | - | |||
3:30 | Add additives | ||||
5:30 | Dump | - | Dump | ||
11:00 | - | Dump | - | ||
second stage | 0:00 | MB from first stage (initial temp.: 50°C) | |||
0:30 | Add curatives | ||||
2:30 | Dump (dump temp.: 80°C 90°C) |