Table 7. Viscoelastic properties of vulcanizates

Compound ENR-25/BR blend ENR-50/BR blend
E25-55 E25-65 E25-75 E50-55 E50-65 E50-75
Tan δ at Tg (DMA, Strain 0.2%) 0.839 0.802 0.726 0.849 0.746 0.648
E” at 0°C (DMA, Strain 0.2%) 4.45 5.18 8.49 16.13 27.55 30.88
Tan δ at 60°C (DMA, Strain 0.2%) 0.083 0.095 0.109 0.100 0.106 0.120
Tan δ at 60°C (DMTS, Strain 5%) 0.099 0.123 0.145 0.125 0.147 0.176